Fault PhenomenonCauses & Corrective Measures
Poor Throwing PowerInsufficient additive content; low cadmium or sulfuric acid concentration; low bath temperature or too low cathode current density.Analyze and adjust bath composition; optimize temperature and current density.
Coarse Deposit GrainExcessive cadmium content; insufficient sulfuric acid; inadequate additives.Replenish additives and adjust bath composition.
Dull Plating DepositLow sulfuric acid concentration and insufficient additives; adjust bath chemical composition.
Pitting on CoatingShortage of OP emulsifier; excess sulfuric acid; excessively high cathode current density.Regulate bath composition and current density.
Brittle Cadmium DepositOver-high cathode current density and excessive gelatin.Reduce current density; perform low-current electrolytic purification.
Turbid Plating SolutionExcess gelatin or β-naphthalenedisulfonic acid.Treat the bath with activated carbon filtration.